Solubility and diffusion of hydrogen in IN-100 and Waspaloy
The solubility of hydrogen, at a fixed hydrogen pressure, was measured in two different heat treatment conditions in both IN-100 and Waspaloy by equilibrium and analysis. The diffusion coefficients were determined by measuring the rate of hydrogen evolution in a vacuum. Hydrogen evolution appeared to be a diffusion-controlled process in all cases. For hydrogen diffusion in Waspaloy, Delta H was 38.5 kJ and D0 was 2.6 x 10 to the -7th sq/s. For IN-100, Delta H was 68.2 kJ and D0 was 59 x 10 to the -7th sq/s. The values for Waspaloy are close to those for pure nickel. The values for IN-100 are more similar to high nickel alloys that show trapping or surface layer impedance.