Standard reference materials: Thermal conductivity of electrolytic iron, SRM 734, from 4 to 300 K
Thermal conductivity data were obtained by the axial one-dimensional heat flow method for a cylindrical rod 3.6 mm in diameter and 23 cm long with an electric heater at one end and a temperature controlled sink at the other. Variability of this iron was studied by means of electrical residual resistivity ratio measurements on 63 specimens. This study showed that with a two-hour anneal at 1000 C one can obtain a thermal conductivity Standard Reference Material that has variability of less than 1% in thermal conductivity.