NASA NTRS1984
The microstructures of commercial VIM-cast and rheocast (Apelian and Cheng, 1983) IN-100 superalloy are investigated optically and by two-stage replica TEM, with an emphasis on the nature of the gamma-prime (GP) precipitates. Photomicrographs at magnifications of 39, 390, 2145, and 6630 are presented and discussed. VIM-cast IN-100 has dendritic structure, 10-20-micron primary GP particles, and uniformly distributed cuboid GP precipitates of a uniform size (about 0.5 micron). Rheocast IN-100 (stirred 20 min at 350 rpm, 1291 C, and 0.0006 torr) has a nondendritic structure, 20-100-micron primary GP particles, and a smaller volume fraction of cuboid GP precipitates with a bimodal (either 1-1.5 microns or less than 0.5 micron) size distribution. Such distribution should increase fatigue-crack-nucleation resistance.