An all-plated, low cost contact system for silicon solar cells
The plating sequences Pd-Cr-Cu and Pd-Ni-Cu are demonstrated. The surface was sensitized with a 50 A-thick Pd layer obtained from an immersion bath. After 15 min heating at 400 C in N2, a thin barrier layer of either Cr or Ni was deposited from electroless baths operated at temperatures around 90 C. The sintering process was repeated, and a thin copper layer of 500 A was deposited by electroless means. An electrolytic copper bath was used to build the copper layer to 3-4 micron thicknesses. Cells with good I-V curves were obtained, and the all-plated contacts had good adhesion. Preliminary cost estimates show that the process costs approximately 12 cents per watt excluding the cost of the masking procedure.