Improved perfluoroalkyl ether fluid development
The feasibility of transforming a commercial linear perfluoroalkylether fluid into a material stable in the presence of metals and metal alloys in oxidizing atmospheres at 300 C without the loss of the desirable viscosity temperature characteristics was determined. The approach consisted of thermal oxidative treatment in the presence of catalyst to remove weak links, followed by transformation of the created functional groups into phospha-s-triazine linkages. It is found that the experimental material obtained in 66 percent yield from the commercial fluid exhibits, over an 8 hr period at 300 C in the presence of Ti(4Al, 4Mn) alloy, thermal oxidative stability better by a factor of 2.6 x 1000 based on volatiles evolved than the commercial product. The viscosity and molecular weight of the developed fluid are unchanged and are essentially identical with the commercial material. No metal corrosion occurs with the experimental fluid at 300 C.