Thermodynamics of aerosols during a molten core-concrete interaction at Fukushima Daiichi Unit 2 estimated conditions
Not Available
Engineering topics
Publications and source records attributed to Grambow, Bernd.
Not Available
Traces of Pu have been detected in material released from the Fukushima Daiichi Nuclear Power Plant (FDNPP) in March of 2011; however, to date the physical and chemical form of the Pu have remained unknown. Here we report the discovery of particulate Pu associated with cesium-rich microparticles (CsMPs) that formed in and were released from the reactors during the FDNPP meltdowns. The Cs-pollucite-based CsMP contained discrete U(IV)O 2 nanoparticles, <~10 nm, one of which is enriched in Pu adjacent to fragments of Zr-cladding. The isotope ratios, 235 U/ 238 U, 240 Pu/ 239 Pu, and 242 Pu/ 239 Pu, of the CsMPs were determined to be ~0.0193, ~0.347, and ~0.065, respectively, which are consistent with the calculated isotopic ratios of irradiated-fuel fragments. Thus, considering the regional distribution of CsMPs, the long-distance dispersion of Pu from FNDPP is attributed to the transport by CsMPs that have incorporated nanoscale fuel fragments prior to their dispersion up to 230 km away from the Fukushima Daiichi reactor site.
The chemical durability of silicate glasses has long been studied for many applications, in particular when glasses are subjected to environmental weathering and aqueous corrosion. Typical applications include optical instruments, glass vessels, radioactive waste confinement, and bone reparation. Glass corrosion involves ion exchange, water diffusion, network dissolution-recondensation, and secondary phase precipitation. These reactions may impact, among other things, the release of contaminants from waste glasses, and the glass mechanical, optical and catalytic properties. The glass corrosion mechanisms and alteration product formation have been well studied as a function of many environmental parameters (temperature, pH, water composition, etc.). The present chapter describes the general phenomena behind glass corrosion and details glass dissolution in aqueous conditions on one hand and glass vapor hydration on the other hand. The latter phenomenon has not received the same level of attention in the literature relative to the corrosion in aqueous solutions. Research and Development needs, in particular in complex systems such as radioactive waste geological repositories, are discussed in the conclusion of the chapter.
The objective of the EC funded GLAMOR project was to achieve a common understanding of the processes that control the decrease of the dissolution rate of high-level waste glass in water when silica becomes saturated. Is affinity control or a protective layer dominating? The following steps were taken: (1) review of the literature, (2) selection ofselect an experimental dataset, and selection of the models r(t) and GM2003, and (3) application apply by the GLAMOR partners of the models to the datasets. The main focus has beenwas on dissolution tests in pure water at different values of surface-to-volume and pH. Some of the main conclusions were: (1) both affinity and protective layer concepts must be considered in the interpretation of the rate decreasing stage, (2) the residual dissolution rate observed beyond the silica saturation stage is far more important in view of the long-term performance of the glass, and deserves more attention in future R&D. In the GLAMOR final report, we also discussed in detail the modeling parameters, such as the silica saturation concentration, the silica diffusion coefficient, the silica retention factor in the reaction layer, and the water diffusion coefficient.
The objective of the EC funded GLAMOR project was to achieve a common understanding of the processes that control the decrease of the dissolution rate of high-level waste glass in water when silica becomes saturated. Is the affinity controlled concept, or the protective layer concept dominating? The following steps were taken: (1) review of the literature, (2) selection of an experimental dataset, and selection of the models r(t) and GM2003, and (3) application by the GLAMOR partners of the models to the datasets. The main focus has been on dissolution tests in pure water at different values of surface to volume and pH. Some of the main conclusions were: (1) both affinity and protective layer concepts must be considered in the interpretation of the rate decreasing stage, (2) the residual dissolution rate observed beyond the silica saturation stage is far more important in view of the long-term performance of the glass, and deserves more attention in future R&D. GLAMOR also discussed in detail the modelling parameters such as the silica saturation concentration, the silica diffusion coefficient, the silica retention factor in the reaction layer, and the water diffusion coefficient.